| Primary Designation | PA6N (Polish standard, e.g., PN-76/H-88021) | D16AT (Russian/Soviet standard, e.g., GOST 4784) |
| International Standards | - EN: EN AW-2017A- AA/ASTM: AA 2017A (less common in US than 2024)- ISO: Al Cu4MgSi(A) | - EN: EN AW-2024- AA/ASTM: AA 2024- ISO: Al Cu4Mg1(A) |
| Similar Grades (Analogues) | - AlCuMg1, 3.1325 (Germany)- A-U4G1 (France)- 2017A (USA/International) | - AlCu4Mg1, 3.1355 (Germany)- A-U4G (France)- 2024 (USA/International) |
| Chemical Composition | - Al: Balance- Cu: 3.5-4.5%- Mg: 0.4-1.0%- Mn: 0.4-1.0%- Si: 0.2-0.8%- Fe: ≤0.7%- Zn: ≤0.25%- Ti: ≤0.15% | - Al: Balance- Cu: 3.8-4.9%- Mg: 1.2-1.8%- Mn: 0.3-0.9%- Si: ≤0.5%- Fe: ≤0.5%- Zn: ≤0.25%- Ti: ≤0.15% |
| Mechanical Properties (T4 Temper) | (Typical values for sheets/plates) - Tensile Strength (UTS): 390-440 MPa- Yield Strength (YS): 250-280 MPa- Elongation: 10-15%- Hardness (Brinell): ~105 HB | (Typical values for sheets/plates) - Tensile Strength (UTS): 440-490 MPa- Yield Strength (YS): 290-340 MPa- Elongation: 10-15%- Hardness (Brinell): ~120 HB |
| Technological Properties | - Machinability: Good, especially in T4 temper. Forms small, brittle chips.- Weldability: Poor with conventional fusion welding (TIG/MIG) due to hot cracking and strength loss in HAZ. Friction Stir Welding (FSW) is better.- Corrosion Resistance: Moderate. Susceptible to intergranular corrosion and stress corrosion cracking in certain environments. Often clad (Alclad) for improved resistance.- Formability: Moderate in T4 temper. Better after annealing. | - Machinability: Excellent, forms brittle chips.- Weldability: Similar to PA6N, poor with conventional fusion welding. FSW preferred.- Corrosion Resistance: Similar to PA6N, moderate. Highly susceptible to intergranular and stress corrosion cracking if not properly protected (e.g., Alclad).- Formability: Moderate. Slightly less formable than 2017A due to higher strength. |
| Heat Treatment | - Solution Heat Treatment: ~495-505°C, followed by quenching.- Aging: Primarily used in naturally aged (T4) condition. Artificial aging (T6) is possible but less common than for 2024. | - Solution Heat Treatment: ~493°C, followed by quenching.- Aging: Most commonly used in naturally aged (T4) or artificially aged (T6, T8) conditions for higher strength. |
| Typical Applications | - Aircraft structures (less critical components)- Rivets- General structural components requiring good strength and machinability- Forgings and heavy-duty parts | - Aircraft fuselage structures, wing tension members, shear webs, ribs- Truck and bus body structures- High-strength aerospace components- Fasteners (rivets) |
| Advantages | - Good strength-to-weight ratio- Good machinability- Relatively good fatigue resistance (compared to other Al alloys) | - Higher strength and fatigue resistance than 2017A/PA6N- Excellent strength-to-weight ratio- Good machinability |
| Disadvantages | - Poor weldability with traditional methods- Moderate corrosion resistance (requires protection)- Lower strength compared to 2024/D16AT | - Poor weldability with traditional methods- Moderate corrosion resistance (requires significant protection, often clad)- Higher cost due to tighter controls and alloying |