This is an excellent question about polymer physics, specifically the glass transition temperature (Tg) and its theoretical explanations. Let me provide a comprehensive explanation of free volume theory and how it relates to the glass transition and mechanical property changes.
Free Volume Theory Overview
Free volume theory was developed primarily by Doolittle and later refined by Fox and Flory. The basic idea is that:
- Total volume of a polymer = occupied volume (by atoms) + free volume (unoccupied space)
- Free volume represents packing defects and holes in the polymer structure
- This free volume is essential for molecular motion
Key Concepts:
1. Free Volume Definition
- Free volume (V_f) = Total volume (V) - Occupied volume (V_occ)
- Fractional free volume (f) = V_f/V ≈ 0.025 at Tg for most polymers
- This is a small but critical amount
2. Temperature Dependence of Free Volume
- Above Tg: Free volume increases significantly with temperature (α_f ≈ 4-8 × 10⁻⁴ K⁻¹)
- Below Tg: Free volume increases very slowly (α_f ≈ 1-2 × 10⁻⁴ K⁻¹)
- This change in thermal expansion coefficient is a defining feature of Tg
3. Connection to Molecular Motion
The critical free volume concept:
- Individual atoms/segments can move when surrounded by sufficient free volume
- When free volume becomes too small (glassy state), segmental motion becomes frozen
- Tg is defined as the temperature where free volume reaches a critical value (~2.5% of total volume)
Transition from Brittle to Rubbery
Below Tg (Glassy State - Brittle):
-
Limited Free Volume: Very little unoccupied space exists
-
Frozen Segments: Polymer chains are locked in fixed conformations
-
Primary Motion Only: Only local group vibrations and rotations possible
-
Stress Response: Stress is accommodated by bond stretching, angle bending, and limited rapid local rotations
-
Energy Dissipation: Low; stress accumulates elastically
-
Mechanical Behavior: High modulus (E ~ 10⁹-10¹⁰ Pa), low strain to failure, brittle fracture with minimal plastic deformation, and high Poisson's ratio approaching 0.5 for incompressible behavior but with constrained deformation
Above Tg, the situation changes dramatically. Increased free volume allows polymer chains to undergo longer-distance conformational changes, enabling segmental motion through crankshaft motions and cooperative movements. Stress now gets accommodated through entire segment reorientation, chain conformational changes, and entropy-driven relaxation, resulting in higher energy dissipation with both elastic and viscous responses. The mechanical behavior shifts to low modulus (E ~ 10⁵-10⁸ Pa), high strain to failure, rubbery elastic behavior, and the ability to undergo large deformations that are partially recoverable.
Crankshaft motion—the coordinated rotation of 2-3 backbone bonds in a manner analogous to an engine crankshaft—represents the fundamental mechanism for generating long-range conformational changes in polymers. This motion requires substantial free volume because atoms must move apart to accommodate the simultaneous rotation of multiple bonds, a spatial demand that exceeds simple single-bond rotation. Below Tg, atomic packing is too tight to permit this coordinated motion, but a critical fractional free volume threshold around 0.025 enables these movements once exceeded.
Segmental motion depends on both thermal energy and available free volume—the probability of motion reflects both the energy barrier to overcome and whether sufficient space exists for the transition state. Doolittle's relationship shows that segmental diffusivity scales exponentially with fractional free volume, meaning as temperature increases and free volume expands, the polymer gains mobility.
Below the glass transition, chains remain kinetically trapped in isolated free volume pockets too small to permit coordinated rotations. At Tg, when free volume reaches its critical threshold, crankshaft motions transition from energetically inaccessible to feasible, bringing segmental relaxation into the experimental timescale. Above Tg, abundant free volume enables these motions to occur readily on picosecond to nanosecond timescales, allowing the chain to explore conformational space.
Once segments can reorient continuously, stress relaxation becomes possible through conformational rearrangement rather than requiring bulk flow. This conformational flexibility is what produces the characteristic lower modulus and rubbery response above the transition. The quantitative picture emerges from the fractional free volume model: above Tg the thermal expansion coefficient is roughly three times larger than below it (αf ≈ 4.8 × 10⁻⁴ K⁻¹ versus αg ≈ 1.48 × 10⁻⁴ K⁻¹), which explains why free volume accumulates so rapidly with temperature once the glass transition is crossed.
The framework also accounts for how molecular weight influences Tg through chain-end effects on free volume distribution, why plasticizers lower Tg by acting as free volume generators, and how applied pressure raises Tg by compressing available free volume. However, the theory has real constraints—it treats all free volume as equally accessible when it isn't, overlooks polymer-specific interactions, and relies on somewhat arbitrary definitions of occupied volume. A complete picture requires combining free volume concepts with configurational entropy considerations and cooperative relaxation dynamics.
Glass Transition via Free Volume Theory
Core Principle: Free Volume as Enabler
Free volume represents unoccupied space in the polymer structure:
Total Volume = Occupied Volume (atoms) + Free Volume (voids/defects)
Fractional Free Volume (f) = V_free/V_total ≈ 0.025 at Tg
At T_g, free volume reaches a critical threshold (~2.5%) below which key molecular motions freeze out.
Brittle (Glassy) → Rubbery Transition
Below Glass Transition (Brittle)
| Aspect | Glassy State |
|---|
| Free Volume | ~0.025 (minimal, tightly packed) |
| Thermal Expansion | α_g ≈ 1.5 × 10⁻⁴ K⁻¹ (slow) |
| Chain Motion | Frozen at segmental level; only bond vibrations possible |
| Stress Response | Elastic deformation only (bond stretching/bending) |
| Properties | E ≈ 10⁹-10¹⁰ Pa; brittle; low strain to failure |
Why brittle? Stress cannot be relieved through chain reorientation—only elastic deformation occurs until bonds break catastrophically.
Above Glass Transition (Rubbery)
| Aspect | Rubbery State |
|---|
| Free Volume | >0.025; increases rapidly with T |
| Thermal Expansion | α_f ≈ 4.8 × 10⁻⁴ K⁻¹ (3× faster!) |
| Chain Motion | Segmental motions enabled; crankshaft rotations possible |
| Stress Response | Dissipated through chain conformational changes (entropic) |
| Properties | E ≈ 10⁵-10⁷ Pa; elastic; high strain recovery |
Why rubbery? Abundant free volume permits chains to reorient, absorbing stress through entropy-driven relaxation rather than molecular bond strain.
Crankshaft Motion & Free Volume Threshold
What is Crankshaft Motion?
A 2-3 bond segment undergoes coordinated rotation:
Before After
W X
| |
A—B—C—D → A—B'—C'—D
| |
X W
This allows long-range conformational rearrangement while minimizing bond energy cost.
Why It Requires Free Volume
Below T_g (f < f_critical):
- Atoms packed densely—attempting crankshaft motion forces atoms into excluded volume
- Energy barrier becomes prohibitively high (atoms must "climb over" neighbors)
- Single bond can rotate, but coordinated 2-3 bond motion is blocked
- Result: Confined motion only (local vibrations)
At T_g Threshold (f ≈ 0.025):
The critical relation emerges:
D∝exp(−fA)
where D is segmental diffusivity and A is a constant.
As f increases toward f_critical:
- Exponent decreases rapidly
- Diffusivity jumps exponentially (10-100× increase)
- Crankshaft motions transition from forbidden → allowed
Above T_g (f > f_critical):
┌─────────────────────────────────────┐
│ Abundant Free Volume │
│ ↓ │
│ B-C-D segment can rotate │
│ while A-B maintains connection │
│ ↓ │
│ Atoms slide past each other │
│ in ns-ps timescale │
└─────────────────────────────────────┘
- Pockets of free volume surround segments
- Coordinated 2-3 bond rotations face minimal steric hindrance
- Crankshaft motions occur frequently (kHz-MHz frequencies)
- Enables stress dissipation through rapid chain reorientation
Quantitative Temperature Behavior
The two distinct thermal expansion regimes reveal the transition:
f_g + \alpha_g(T - T_g) & T < T_g \\
f_g + \alpha_f(T - T_g) & T > T_g
\end{cases}$$
**Example:** PMMA at T_g ≈ 378 K
```
At 350 K (below T_g): f ≈ 0.0235, slow molecular motion
At 378 K (at T_g): f ≈ 0.0250, crankshaft motions emerge
At 420 K (above T_g): f ≈ 0.0275, crankshaft motions frequent
```
The **~3-fold difference** in thermal expansion (α_f/α_g ≈ 3) above vs. below T_g is diagnostic—at T_g, the polymer's heating simultaneously adds free volume AND permits previously forbidden motions.
---
## Physical Picture: Why Crankshaft Motion Changes Everything
| Process | Energy Scale | Free Volume Requirement |
|---------|-------------|----------------------|
| Local C-C vibration | ~1 kT | None (happens always) |
| Single bond rotation | ~3 kT | Minimal (side chains can move aside) |
| **Crankshaft (2-3 bonds)** | **~5-8 kT** | **f > 0.025 (critical!)** |
| Full chain reptation | ~100 kT | Full liquid state |
Crankshaft motion is the **minimum cooperative motion** enabling stress relaxation. Below T_g, stored elastic energy cannot be released through conformational averaging—only through catastrophic bond rupture (brittle fracture).
---
## Connection to Plasticizers & Pressure
- **Plasticizers** (e.g., dibutyl phthalate) increase f → *lower* T_g ✓
- **Pressure** decreases f → *raises* T_g ✓
- **Cross-linking** restricts crankshaft motions → *raises* T_g ✓
All consistent with free volume framework.